Calcined Alumina And Refractories

Jul 15, 2022

Sufficient fine grinding of the α-Al2O3 aggregates can destroy their aggregated state and make them non-porous primary crystals, at which time the particle size means close to its grain size. Activated alumina is calcined alumina that has been sufficiently finely ground and has α-Al2O3 with an original crystal size of less than 1 μm as the basic composition (20% to >90%). In the production of activated alumina, strong grinding is usually required, such as dry grinding in a ceramic-lined ball mill with ceramic balls as the grinding medium for more than 24 hours. The reason why it is called activated alumina usually means that it is easy to achieve the highest sintering density when sintered, but the sintering temperature is 100-200 °C lower than that of the low-activity α-Al2O3 powder; It is easy to react and sinter with other components in the material matrix, such as combining with clay in the matrix to form mullite, reacting with calcium aluminate cement to form CA6, reacting with MgO to form spinel, etc. According to the sintering theory, the grain size greatly affects the sintering rate in the initial stage, that is, the formation and growth of the neck between the grains. If the grain size is reduced to 1/10 of the original size (eg from 5 μm to 0.5 μm), sintering will be 1000 times to 10000 times easier. This explains the high thermal activity of activated alumina.

The grinding process consumes a lot of energy, so the finer the powder, the more expensive it is. The appearance of silicon micro (the foggy SiO2 generated during the production of silicon carbide or silicon metal) has greatly contributed to the development of low-moisture, low-cement and ultra-low cement castables, but this active SiO2 also limits the castables. Operating temperature. If there is no successful development of activated alumina, the modern refractory castable industry cannot develop so rapidly, and the operating temperature will not exceed 1600 ℃.

 Generally speaking, powders can be divided into two categories according to the shape of particle size distribution (PSD for short): one type has a unimodal PSD, that is, the particle size distribution curve only surrounds a special particle size (close to but not necessarily Yes D50) peak: the other type is the PSD with multi-peak, that is, there are two or more distribution peaks on the PSD curve. Whether it is unimodal or bimodal, generally the wider the PSD range, the greater the powder bulk density or green body density. The PSD powder with unimodal and narrow range has the lowest bulk density. Of course, activated alumina also has the above two types. The unimodal activated alumina is characterized by a higher percentage (>80%) of particles <1μm (≈primary crystal size), and thus has a higher activity, and the average value of their particle size (≈grain size) is 0.30. around 5μm. The density of this activated alumina green body is low, usually only 54% 55% of the theoretical density of α-Al2O3 (3.98g/cm3), but its density after firing at 15001600 ℃ can reach 98% of the theoretical density, or even higher. Unimodal activated alumina is easily and completely dispersed in water with the aid of dispersants such as sodium polyphosphate. The content of active particles smaller than 1 μm in the multi-bee activated alumina varies greatly. Usually between 20% and 7O%. The ratio of the number of active particles to the number of larger particles (>1 μm) determines its void-filling ability and activity. For multimodal activated alumina, the median diameter D50 can only represent its fineness, rather than a parameter that characterizes its properties. The green density of multimodal activated alumina can usually reach 62%68% of the theoretical value, which is obviously higher than that of unimodal activated alumina. The sintered density that multimodal activated alumina can achieve depends on its activity. When the higher activity multimodal alumina is used for pressing and sintering, although its sintering temperature is 100-150 °C higher than that of the fully densified unimodal activated alumina, its sintered density is only 94% and 96% of the theoretical value. The particles are easily detached from the larger particles, so the multimodal activated alumina is easy to disperse in water. The wide range of PSD of the multimodal activated alumina enables the α-Al2O3 micropowder to be filled into the gaps between the aggregates of the refractory bricks and the castables and the remaining voids between the large powder particles. Therefore, when used in castables, to achieve the same fluidity, the amount of water added can be reduced by 4% and 5%. In the matrix of the castable, the multimodal activated alumina acts as a lubricant between the large particles, which can minimize the loosening of the castable, even when subjected to intensive mixing or pumping. keep separate from each other.